Zirconium 702 (UNS R60702) vs Zirconium 705 (UNS R60705) — Complete Comparison
Under ASTM B551, Zirconium 705 (Zr-2.5% Nb, UNS R60705) delivers 85% higher minimum yield strength than commercially pure Zirconium 702 (380 MPa vs. 205 MPa), enabling thinner high-pressure reactor walls—but Zr 705 mandates post-weld stress-relief heat treatment to prevent delayed hydride cracking, whereas Zr 702 offers slightly higher corrosion immunity and simpler as-welded fabrication.
| Property | Zirconium 702 (UNS R60702) | Zirconium 705 (UNS R60705) |
|---|---|---|
| UNS & Composition | R60702 (Zr+Hf >= 99.2%) | R60705 (Zr + 2.0–3.0% Nb) |
| Min Tensile Strength (ASTM B551) (MPa) | 380 (55 ksi) | 550 (80 ksi) ★ |
| Min Yield Strength (0.2%) (MPa) | 205 (30 ksi) | 380 (55 ksi) ★ |
| Min Elongation (in 50 mm) (%) | 16 | 16 |
| Post-Weld Heat Treatment (PWHT) | Generally not required ★ | Mandatory stress relief (~550–595°C) |
| Corrosion Resistance (Extreme H₂SO₄) | Best (unalloyed single-phase) ★ | Very Good (slightly narrower ceiling) |
| Bend Radius / Deep Drawing | Better for complex forming ★ | Good (higher springback) |
| Typical Equipment Application | Heat exchanger tubes, vessel liners, columns | High-pressure reactors, shafts, bolts, pumps |
Choose Zirconium 702 (UNS R60702) When
- ✓ Heat exchanger tubes, distillation columns, and corrosion-resistant liners
- ✓ Field-welded piping where furnace post-weld stress relief is impractical
- ✓ Maximum corrosion safety margin in boiling H2SO4 or concentrated HCl
- ✓ Complex cold forming, spinning, or tube expansion
Choose Zirconium 705 (UNS R60705) When
- ✓ High-pressure ASME reactors where 85% higher yield strength cuts wall thickness
- ✓ Zirconium fasteners, pump shafts, agitator blades, and structural internals
- ✓ Shop-fabricated assemblies with access to vacuum or inert-gas PWHT furnaces
- ✓ Reducing total zirconium tonnage in thick-wall pressure shells
Engineering Trade-Off Analysis: Zirconium 702 (UNS R60702) vs. Zirconium 705 (UNS R60705)
Niobium Alloying & Mechanical Design Stress: Zirconium 702 contains >=99.2% Zr+Hf and is the workhorse for standard chemical equipment. Adding 2.0–3.0% niobium in Zirconium 705 raises minimum tensile strength from 380 MPa to 550 MPa and minimum yield strength from 205 MPa to 380 MPa while maintaining >=16% elongation—substantially boosting ASME Section VIII allowable design stresses.
The Mandatory Post-Weld Stress Relief Rule for Zr 705: Both grades require immaculate cleaning and trailing argon shielding during GTAW welding. However, welds in Zirconium 705 form a martensitic-like alpha-prime structure in the heat-affected zone that is prone to delayed hydride cracking and stress corrosion in acid service unless stress-relieved at ~550–595°C (1025–1100°F) within 14 days of welding. Zr 702 is routinely placed into service as-welded.
Corrosion Nuance in Ultra-Aggressive Acids: In most HCl, acetic, and nitric acid streams, Zr 702 and Zr 705 perform similarly. However, in borderline hot concentrated sulfuric acid (>65–70%) or nitric acid near stress-corrosion thresholds, unalloyed Zr 702 maintains the cleanest single-phase resistance and better tight-radius cold formability.
Related Specifications, Grades & Mill Products
Frequently Asked Questions: Zirconium 702 (UNS R60702) vs Zirconium 705 (UNS R60705)
Why does ASTM B551 Zirconium 705 require post-weld stress relief when 702 does not?
Does Hafnium (Hf <= 4.5%) affect chemical corrosion resistance in Zr 702 or Zr 705?
Not sure which material is right for your project?
Our engineers can recommend the optimal grade based on your specific application, environment, and budget requirements.
Related Comparisons
Grade Comparison
Grade 2 (CP Titanium) vs Grade 5 (Ti-6Al-4V)
Grade Comparison
Grade 5 (Ti-6Al-4V) vs Grade 23 (Ti-6Al-4V ELI)
Grade Comparison
CP Titanium (Grade 1-4) vs Titanium Alloys (Grade 5, 9, 23)
Grade Comparison
Titanium Grade 7 (Ti-0.15Pd) vs Titanium Grade 12 (Ti-0.3Mo-0.8Ni)
Grade Comparison
TA15 / GOST VT20 (Ti-6.5Al-2Zr-1Mo-1V) vs Grade 5 (Ti-6Al-4V)